ABS - Acrylonitrile-butadiene-styrene
| Processing Guide: | ABS - Acrylonitrile-butadiene-styrene |
| Extruder: | Single screw, no vacuum, grooved feeding section |
| Screw Design: | Barrier screw 25 - 30 L/D |
| Compression Ratio: | 2,75 : 1 |
| Cylinder Temperatures: | 190-240 C 374-464 F |
| Melt Temperature: | 200-245 C 392-473 F |
| Pre-Drying: | 3 hours at 70-80 C (158-176 F) |
| Calibration: | |
| Miscellaneous: | approx. 30 % higher torque (than PVC) |
| Note: This is meant as a general guide. Please consult your material and machinery representative. |