PVC-C - Polyvinylchloride chlorinated
| Processing Guide: | PVC-C - Polyvinylchloride chlorinated |
| Extruder: | Twin screw extruder with vacuum, plain feeding section |
| Screw Design: | Four stage PVC screw (low-shear screw) three start precompression section 25 - 30 L/D |
| Compression Ratio: | 1,7:1 |
| Cylinder Temperatures: | 180-195 C 356-383 F |
| Melt Temperature: | 180-195 C 356-383 F |
| Pre-Drying: | no |
| Calibration: | |
| Miscellaneous: | more sensitive to heat and shear than PVC, output only approx. half of PVC-U |
| Note: This is meant as a general guide. Please consult your material and machinery representative. |