Processing Guide:
|
PC - Polycarbonat
|
 |
|
Extruder:
|
Single Screw (profile, sheet, film ) without vacuum , plain feeding section with vacuum or pressure-relieved grooved feeding section (by increased screw pitch and channel depth) Twin Screw (compounding)
|
 |
|
Screw Design:
|
Barrier Screw, 25 - 30 L/D
Two mixing sections: dispersive-mixing spiral-shear element, rhomboid distributive-mixing section
|
 |
|
Compression Ratio:
|
2,25:1
|
 |
|
Cylinder Temperatures:
|
270-300 C 518-572 F
|
 |
|
Melt Temperature:
|
290-320 C 554-608 F
|
 |
|
Pre-Drying:
|
2-4 hours at 100-120 C (212-248 F)
|
 |
|
Calibration:
|
|
 |
|
Miscellaneous:
|
should not succeed 400 C reduced wear by preheating of material at 120 C (248 F) or by heating of feeding section at 170 C (338 F)
|
|