PA 66 - Polyamide 66
Processing Guide: | PA 66 - Polyamide 66 |
![]() |
|
Extruder: | Single Screw Extruder Without vacuum, plain feeding section |
![]() |
|
Screw Design: | Barrier Screw or Polyolefin Screw with equal feed ,transition and metering section, 25-30 L/DTwo mixing sections: dispersive-mixing spiral-shear element, rhomboid distributive-mixing section |
![]() |
|
Compression Ratio: | 3-4:1 |
![]() |
|
Cylinder Temperatures: | 260-290 C 500-554 F |
![]() |
|
Melt Temperature: | 280-300 C 536-572 F |
![]() |
|
Pre-Drying: | 3 hours at 80 C (176 F) (very important) |
![]() |
|
Calibration: | |
![]() |
|
Miscellaneous: | process above 250 oC (482 F) to avoid freeze-off if bubbles come then temperature too high increased output/reduced wear by preheating of material 75 C (167 F) or by heating of feeding section at 160 C (320 F) |
Note: This is meant as a general guide. Please consult your material and machinery representative. |