PC - Polycarbonat
Processing Guide: | PC - Polycarbonat |
![]() |
|
Extruder: | Single Screw (profile, sheet, film ) without vacuum , plain feeding section with vacuum or pressure-relieved grooved feeding section (by increased screw pitch and channel depth) Twin Screw (compounding) |
![]() |
|
Screw Design: | Barrier Screw, 25 - 30 L/DTwo mixing sections: dispersive-mixing spiral-shear element, rhomboid distributive-mixing section |
![]() |
|
Compression Ratio: | 2,25:1 |
![]() |
|
Cylinder Temperatures: | 270-300 C 518-572 F |
![]() |
|
Melt Temperature: | 290-320 C 554-608 F |
![]() |
|
Pre-Drying: | 2-4 hours at 100-120 C (212-248 F) |
![]() |
|
Calibration: | |
![]() |
|
Miscellaneous: | should not succeed 400 C reduced wear by preheating of material at 120 C (248 F) or by heating of feeding section at 170 C (338 F) |
Note: This is meant as a general guide. Please consult your material and machinery representative. |